Standar Lingkungan EU 2.0 Nyuwun manawa konten timah (PB) kurang saka 1000ppm.basing iki, Kinkou ngembangake C17300 sing murah lan kinerja nglereni kanthi C17300.Kinkou uga nyedhiyakake campuran tembaga gratis Waca rangkeng-. Kinerja nglereni C17200 iki uga apik.

1. Komposisi kimia saka Low C17300

Model

Be

Ni + co

Ni + co + fe

Pb

Cu

C17300

1.8-2.0

≥0.20

≤0.6

<0.1

Snang

2. Sifat fisik lan mekanik sakapimpinan sithikC17300

Negara
(Miturut ASTM)

Perawatan Panas
(℃)

Diameteripun

(mm)

Kekuwatan tensile (MPA)

Kekuwatan Ngasilake (MPA)

Elongasi

4xd (%)

Hardness

Konduktivitas listrik

(IAC,%)

HV0.5

HRB utawa HRC

TB00

775 ℃ ~ 800 ℃

Kabeh

410-590

> 140

> 20

159-162

B45-b85

15-19

Td04

775 ℃ ~ 800 ℃ Solusi + Proses Dingin Hardening

8-20

620-860

> 520

> 8

175-257

B88-B102

15-19

0,6-8

620-900

> 520

> 8

175-260

B88-B103

Th04

315 ℃ x1 ~ 2hr

8-20

1140-1380

> 930

> 20

345-406

C27-C44

23-28

0,6-8

1210-1450

> 1000

> 4

354-415

C38-C45